Been using prusaslicers default PLA profile with issues and this is my first roll of PETG, so I just selected the corresponding profile for that.

It seems so be super stringy whenever there’s movement and when printing the bunny (in vase mode) there’s lots of holes in the model.

I’m not sure if this is an issue with calibration (didn’t do anything when switching from PLA) or if the filament is wet.

  • SymbioteSynapse@lemmy.world
    link
    fedilink
    English
    arrow-up
    5
    ·
    1 year ago

    Check for a partial clog. 80% of the time i get that consistency with petg, its because the nozzle is partially clogged. The other 20% is the ptfe tubing is shot. Usually it partially melts and causes underextrusion.

    Wet filament could be an issue too, but this is pretty extreme for wet filament.

    • drudoo@lemmy.worldOP
      link
      fedilink
      English
      arrow-up
      1
      ·
      1 year ago

      You were right! All clogged up.

      Replaced the nozzle, heat block (heating element, sensor, PTFE) and fan duct. Wasn’t able to unscrew the nozzle (got stuck 80% out) so I replaced the whole thing.

      Did two new temp towers:

      Left tower is 235 (top) to 260 (layers labeled 280-260 are all 260). Right is 220-240.

      https://i.imgur.com/1MQkStE.jpg

      https://i.imgur.com/HDWq19A.jpg

      I definitely feel like 220 is the right temp for this.

      • SymbioteSynapse@lemmy.world
        link
        fedilink
        English
        arrow-up
        1
        ·
        1 year ago

        Make sure you calibrate your e-steps after swapping hotends. I did the same thing on my ender 3 putting on a volcano hotend, and started getting overextrusion. After adjusting the e-steps it was back to normal.